Photon energy | 1486.61eV |
Spectrum type | Au 4f |
Resolution | 20 |
Dwell Time | 0.1 |
Step size | 0.1 |
Number of scans | 30 |
Name | 2. Au in 25mBar O2 |
Ex situ preparation | Sample mounted on a stainless steel holder using stainless steel clips. |
In situ preparation | Sputter cleaned for 15 minutes using 3 kV Ar at a pressure of 1E-5 and 10 mA emission current. |
Additional Information | Au foil measured in 25 mbar O2. |
Measurement Date | 28-08-2020 |
Condition | Value | Units |
---|---|---|
pressure | 25 | mbar |
temperature | 25 | C |
ambient composition | O2 | none |
Analyzer Mode | FAT |
Area | 0.3 mm diameter |
Strength | 100 W, 15 kV |
Source Beam Size | 0.3 mm diameter |
Take Off Angle | 90 degrees |
Analyzer Acceptance Angle | 22 degrees |
Laboratory | Surface Analytics |
Instrument | Phoibos NAP-150 |
Protocol | ISO 15472:2010 |
Calibration date | 06-02-2020 |
Binding Energy | 83.96 |
Emission line | Au 4f7/2 |
Binding Energy | 932.64 |
Emission line | Cu 2p3/2 |